Soft Magnetic Alloy yeShielding uye permalloy musimboti

Product Detail

soft-magnetic-alloy-foil

Soft Magnetic Alloy : imhando yealloy ine yakakwira permeability uye yakaderera kumanikidza mune isina simba remagineti.Rudzi urwu rwealloy runoshandiswa zvakanyanya muindasitiri yemagetsi eredhiyo, chaiyo chiridzwa, kuremote control uye otomatiki kudzora masisitimu.Pamwe chete, inonyanya kushandiswa muzvikamu zviviri: simba rekushandura uye kugadzirisa ruzivo.Chinhu chakakosha muhupfumi hwenyika.

Fe-Ni Soft Magnetic Alloy                                                                                                                                                                             

Giredhi:1J50 (Permalloy), 1J79(Mumetal,HY-MU80), 1J85(Supermalloy),1J46

Standard: GBn 198-1988
Application: Zvizhinji zvezvidiki zvinoshandura, pulse transformers, relays, transformers, magnetic amplifiers, electromagnetic clutches, chokes iyo inoshandiswa kune isina simba kana yepakati magineti minda Inoyerera mhete core uye magineti nhovo.

 

Ronga

Giredhi

Composition

International Similar Giredhi 

IEC

Rashiya

USA

UK

Yakakwira yekutanga permeability yeakapfava magineti alloy

1J79

Ni79Mo4

E11c

79НМ

Permalloy 80 HY-MU80

Mumetal

1J85

Ni80Mo5

E11c

79НМА

Supermalloy

-

Yakakwira magineti conductivity yakakwira saturation magineti flux density yakapfava magineti alloy

1J46

Ni46

E11e

46Н

45-Permalloy

 

1J50

Ni50

E11a

50Н

Hy-Ra49
Permalloy

Radiometal

Chemistry yeFe-Ni Soft Magnetic Alloy

Giredhi

Muumbi weKemikari(%)

 

C

P

S

Mn

Si

Ni

Mo

Cu

Fe

1J46

0.03

≤0.02

≤0.02

0.6-1.1

0.15-0.30

45-46.5

-

≤ 0.2

Bal

1J50

0.03

≤0.02

≤0.02

0.3-0.6

0.15-0.30

49-50.5

-

≤ 0.2

Bal

1J79

0.03

≤0.02

≤0.02

0.6-1.1

0.30-0.50

78.5 -81.5

3.8- 4.1

≤ 0.2

Bal

1J85

≤0.03

≤0.02

≤0.02

0.3-0.6

0.15- 0.30

79- 81

4.8- 5.2

≤ 0.2

Bal

Mechanical Property :

Giredhi

Resisitivity
(μΩ•m)

Desinty (g/cm3)

Curie Point

Brinellhardness
HBS

σbTensile
Simba
MPa

σsYield Simba
MPa

Elongation
(%)δ

Un-annealed

1J46

0.45

8.2

400

170

130

735

 

735

 

3

 

1J50

0.45

8.2

500

170

130

785

450

685

150

3

37

1J79

0.55

8.6

450

210

120

1030

560

980

150

3

50

1J85

0.56

8.75

400

-

-

-

-

-

-

-

-

Yakakwira saturation magineti induction yakapfava magineti alloy                                                                                                               

Giredhi:1J22 (Hiperco 50)

Standard:GB/T15002-94
Application: Electromagnetic Ji musoro, nharembozha diaphragm, torque mota rotor.

Rashiya USA UK Furanzi Janpane
50KΦ Supermendur
Hiperco 50
Permendur AFK502 SME SMEV

Chemical Compostations:

C Mn Si P S Cu Ni Co V Fe
MAX(
0.025 0.15 0.15 0.015 0.010 0.15 0.25 47.5-49.5 1.75-2.10 BAL

Mechanical Property :

Denstiy
(Kg/m3
(g/cm3
Resisitivity
(μΩ•mm(μΩ•cm
Curie Poin( Magnetic coefficient (10-6 Saturation Magnetic(T(KG Elastic Modulus
(GPA/psi
Thermal Conductivity
(W/m·K/cm·s℃
8 120(8.12 400(40 940 60 2.38(23.8 207(x103 29.8(0.0712

Coefficient of Linear Expansion/(10-6/°C)

20-100 ℃ 20-200 ℃ 20-300 ℃ 20-400 ℃ 20-500 ℃ 20-600 ℃ 20-700 ℃ 20-800 ℃
9.2 9.5 9.8 10.1 10.4 10.5 10.8 11.3

Magnetic Performance

Mafomu Dimension/(mm/in Minimum flux density/yeanotevera magineti intensitiesT(KG
800 A/m
10Oe
1.6KA/m
20Oe
4KA/m
50Oe
8KA/m
100Oe
Strip   2.00(20.0 2.1(21.0 2.20(22.0 2.25(22.5
Bar 12.7-25.4(0.500-1 1.60(16.0 1.80(18.0 2.00(20.0 2.15(21.5
Rod >12.7(1 1.50(15.0 1.75(17.5 1.95(19.5 2.15(21.5